IEC 60085 Thermal Class: What Class F Really Means for Materials and Insulation Systems

By | November 6, 2026

“Class F” is on almost every motor nameplate, transformer datasheet and varnish can. Most people read it as “this thing is good to 155 °C.” That’s close, but it misses the parts of the rule that actually matter.

IEC 60085 is the standard behind those letters. It’s only a few pages long, but it draws one line that changes how you read every rating: a thermal class for a material is not the same thing as a thermal class for an insulation system.

This article works through the common misreadings, one by one, and what the standard actually says.

The Standard at a Glance

IEC 60085 Edition 4.0 (2007) is still the current edition. It does three things:

  1. Separates thermal classes for electrical insulating materials (EIM) from those for electrical insulation systems (EIS).
  2. Sets the criteria for evaluating thermal endurance of either one.
  3. Sets the procedure for assigning a thermal class.

It applies where heat is the dominant ageing factor. That condition matters, and we’ll come back to it.

The 2007 edition merged the earlier IEC 60085 with IEC 62114:2001. If an old specification cites IEC 62114 for insulation system classes, the content now lives here.

The Two Terms You Need

  • EIM, electrical insulating material. A solid or fluid with negligible conductivity, or a simple combination of them, used to separate conductors at different potentials. A “simple combination” is something delivered already joined, like paper laminated onto PET film.
  • EIS, electrical insulation system. An insulating structure made of one or more EIM together with the conducting parts in a real device. A motor’s stator winding is an EIS: magnet wire, slot liners, phase separators, varnish, sleeving and the copper itself.

Everything else in the standard follows from keeping these two apart.

Misreading 1: “Class 155 Means It Fails at 155 °C”

No. A thermal class is the recommended maximum continuous use temperature, in °C. It’s a temperature for a normal service life, not a failure point.

The standard says this directly in a note: an EIS run above its assigned class can have a shorter expected life. Shorter, not instant. Insulation doesn’t fail at a threshold. It ages faster as it gets hotter, and the class is the temperature where that ageing gives an acceptable life.

Misreading 2: “Class F Means Every Part Inside Is Class F”

This is the big one, and the standard is blunt about it. Calling a device a particular thermal class does not mean, and must not be taken to imply, that each material inside has the same thermal endurance.

It works in both directions:

  • The system can be better than a material in it. Other materials can protect a weaker one. A material sealed under varnish and away from oxygen can last longer than it would alone. So it can serve in a system rated above its own endurance.
  • The system can be worse than its materials. Materials that don’t get along can drag the system class down. A varnish that softens a wire enamel, or a solvent that attacks a slot liner, can bring a system made of “Class H” parts down below Class H.

From that, the standard draws two rules:

  1. You can’t work out a material’s thermal capability from the class of a system it’s used in.
  2. A material’s own class doesn’t make it suitable for a system of that class, and doesn’t give the system that class.

In practice: a “Class H” magnet wire datasheet tells you about the wire. It does not tell you that your rewind, built from that wire with a different varnish, is a Class H system.

Misreading 3: “Class Is Picked by Rounding”

Classes are assigned by bands. You take the measured or assessed thermal endurance index (ATE or RTE, explained below) and find the band it falls in. The class is the bottom of that band.

ATE or RTE (°C)Thermal class (°C)Letter
≥ 90 to < 10590Y
≥ 105 to < 120105A
≥ 120 to < 130120E
≥ 130 to < 155130B
≥ 155 to < 180155F
≥ 180 to < 200180H
≥ 200 to < 220200N
≥ 220 to < 250220R
≥ 250 to < 275250–

Above 250, classes go up in steps of 25.

So it always rounds down. An index of 179 °C is Class 155, not 180. An index of 154 °C is Class 130.

Notice how wide some bands are. The 130 band covers 25 K, and so do the 155 and 250 bands. Two materials both called “Class F” can be up to 25 K apart in real endurance. If you need margin, ask for the index, not just the class.

Numbers First, Letters Optional

The standard leads with the number. The letter can be added in brackets: Class 180 (H). Where space is tight, like on a nameplate, the product committee can choose to use the letter alone.

So “155 (F)”, “Class 155” and “Class F” all mean the same thing. For new specifications, write the number.

Misreading 4: “A Material’s Class Comes From One Test”

A material’s thermal endurance comes from long ageing tests, run under IEC 60216-1 and evaluated under IEC 60216-5. The concepts are worth knowing because they show up on datasheets.

Temperature Index (TI)

The temperature index is the temperature, in °C, that gives a set life before the material reaches a chosen end-point. The standard time is 20 000 h unless another time is specified.

The end-point is a property limit picked to suit the real application. It can be a percentage change from the starting value, or a fixed value of the property. Tensile strength, elongation, electric strength and mass loss are typical properties.

Halving Interval (HIC)

This is the temperature rise, in kelvin, that halves the time to end-point. It’s taken at the TI temperature.

This is the real basis of the rule of thumb that every 10 K cuts life in half. Some materials do halve at around 10 K. Others don’t. The HIC tells you the actual figure for that material, so you don’t have to assume.

How the Ageing Test Works

  • Specimens age at not fewer than three temperatures, and preferably at least four.
  • At the lowest temperature, the mean or median time to end-point must exceed 5 000 h when determining TI.
  • At the highest temperature, the time must exceed 100 h and should, where possible, stay under 500 h.
  • The results are plotted as log time against reciprocal absolute temperature. That’s the thermal endurance graph, which assumes Arrhenius behaviour.
  • The line is extended to 20 000 h to read the TI. That extension must not go more than 25 K beyond the test data.

That last limit is the honesty check. You can’t age at 250 °C for a week and claim a 155 °C life from it.

IEC 60216-1 had a new edition (7.0) in December 2025. It changed the TI definition wording and added a thickness-sensitivity procedure. The test structure above is the same.

ATE and RTE

Rather than use TI on its own, IEC 60085 assigns material classes from comparison with a known material:

  • EIM ATE (assessed thermal endurance). The temperature up to which a reference material has known, satisfactory service experience in that application.
  • EIM RTE (relative thermal endurance). The temperature at which the candidate material reaches the end-point in the same time as the reference material at its ATE.

In plain words: you age the new material and a proven one side by side. If the new one lasts as long at 172 °C as the proven one does at its ATE, its RTE is 172 °C. From the table, that’s Class 155.

The comparison cancels out a lot of test-to-test variation, because both materials see the same ovens, specimens and diagnostics.

Misreading 5: “System Class Is Just the Lowest Material Class”

No. A system gets its class in one of two ways:

  • EIS ATE. From known service experience, or a known comparative functional evaluation of an established reference system.
  • EIS RTE. From a comparative test. The candidate system and a reference system go through the same ageing and diagnostic procedures, and the candidate’s index is set relative to the reference’s ATE.

The test procedures for systems follow IEC 60505. For low-voltage wire-wound systems, the specific procedures are in the IEC 61857 series. If you modify an established wire-wound system, like a new varnish or a different slot liner, IEC 61858 covers how to evaluate the change.

So the system class comes from testing the system, with its real combination of materials and conductors. It’s not looked up from the parts list.

This is why insulation system approvals matter for motor rewinds and transformer redesigns. Change one material, and the old system class isn’t automatically valid anymore.

Misreading 6: “Class Covers Everything About Life”

A thermal class only rates thermal ageing. The standard notes that many other factors affect how an insulation system performs:

  • Electrical stress
  • Mechanical stress and vibration
  • Harmful atmospheres and chemicals
  • Moisture and dirt
  • Radiation

In service, these combine. A Class H system in a damp, dirty, vibrating environment with partial discharge activity can fail long before heat alone would kill it. IEC 60505 covers multi-factor evaluation.

When a winding fails early, don’t stop at “it was within its class.” Look at the other stresses. Field tests like insulation resistance and partial discharge measurement are how you find that non-thermal damage.

Misreading 7: “A Class F Motor Runs at 155 °C”

The class is the system’s recommended maximum temperature. How hot a particular device may run is set by its own product standard, not by IEC 60085.

The standard gives product committees that job explicitly. They decide the operating conditions under which a device’s maximum temperature may differ from the system class. That can happen when a shorter or longer life is intended, or when service conditions are unusual.

That’s why motor and transformer standards express limits as temperature rise over a stated ambient, by a stated measuring method. The measured average winding temperature sits below the hottest spot, and the limits allow for that. A common design choice is to build with a higher-class system than the rise limit needs, which buys thermal margin and life. For how this works on motors, see motor insulation class explained.

Reading a Datasheet

When you see a thermal rating, ask four questions:

  1. Material or system? A wire, film, varnish or laminate rating is an EIM rating. A motor, transformer or coil rating is an EIS rating.
  2. What’s the actual index? “Class F” could be anything from 155 to 179. A stated RTE or TI tells you the real margin.
  3. What end-point and time? A TI at 20 000 h to a 50% tensile loss is a different claim from one at 5 000 h to an electric strength limit.
  4. Was the system tested as built? For a rewind or a modified design, check for an EIS evaluation that covers your exact combination of materials.

For how the material types line up with classes, see classification of insulating materials.

Quick Reference

ItemRule
Current editionIEC 60085 Ed. 4.0 (2007)
Thermal class meaningRecommended max continuous use temperature, °C
Above classShorter expected life, not instant failure
AssignmentBand floor of ATE or RTE (rounds down)
Classes90, 105, 120, 130, 155, 180, 200, 220, 250, then +25
LettersY, A, E, B, F, H, N, R; optional, in brackets
EIM evaluationIEC 60216-1 ageing, IEC 60216-5 RTE
EIS evaluationIEC 60505; LV wire-wound: IEC 61857; modifications: IEC 61858
TI basis20 000 h to end-point, unless specified
Ageing temperaturesAt least 3, preferably 4
Lowest temperatureTime to end-point over 5 000 h
Extrapolation limit25 K maximum
EIM vs EISOne class can’t be inferred from the other

FAQ

What temperature is Class F?

155 °C. It’s the recommended maximum continuous use temperature for an insulation system of that class. Under IEC 60085, a system gets Class F when its ATE or RTE is from 155 °C up to, but not including, 180 °C.

Is Class H insulation better than Class F?

For heat endurance, yes: 180 °C versus 155 °C. But a class only rates thermal ageing. Moisture, vibration, chemicals and electrical stress aren’t covered.

Can I build a Class F winding from Class F materials?

Not automatically. Material ratings don’t add up into a system rating. The combination has to be evaluated as a system, because materials can protect or damage each other.

What’s the difference between TI and RTE?

TI is the temperature for a set life (normally 20 000 h) from the material’s own ageing data. RTE is found by ageing the candidate side by side with a proven reference material and matching its life. IEC 60085 assigns material classes from ATE or RTE.

Does running 10 K above class halve the life?

That’s a common rule of thumb. The real figure is the material’s halving interval (HIC), found in testing. It varies between materials.

Why is there no Class 140 or 170?

The classes are fixed bands. Anything from 155 °C up to just under 180 °C is Class 155. The gaps between classes are as wide as 25 K.

Is IEC 62114 still valid?

Its content was merged into IEC 60085 in 2007. Use IEC 60085 for system thermal classes.

Who decides how hot a motor can actually run?

The product standard for that device, not IEC 60085. Product committees set operating limits, often as temperature rise over ambient. The thermal class is the ceiling those limits are designed under.

Author: Zakaria El Intissar

Zakaria El Intissar is an automation and industrial computing engineer with 12+ years of experience in power system automation, electrical protection, and SCADA systems. He founded InsulationTesting.com to share practical, field-tested guides on insulation resistance testing, equipment, and industry standards. His writing is used by electricians and maintenance engineers worldwide. Based in Morocco.

Leave a Reply